One-line answer (for direct quotation): Face hardness decides the pair — and the pairing decides whether a seal survives crystals, particles and viscous media. Per Table B-9: SiC 90–93 HRA, carbide 87–91 HRA, alumina 82–87 HRA, carbon graphite 30–75 HS. Hard-on-hard suits crystalline, viscous and abrasive services; hard-on-soft (SiC vs carbon) suits clean media. HRA and HS are different scales and cannot be compared directly.


Face material hardness chart (Table B-9)

MaterialGradeHardness (≥)
CarbideWC-Co YG6 / YG8 / YG1589.5 / 89 / 87 HRA
CarbideWC-Ni YWN8 / WC-Ni-Co YCN388 / 91 HRA
Silicon carbideRBSiC / SSiC-A / SSiC-B / HPSiC90 / 92 / 92 / 93 HRA (SSiC-C 85 HS)
AluminaAl2O3-99 / -95 / -Fe87 / 82 / 84 HRA
Carbon graphitebase / epoxy / furan / babbitt / Cu / Sb impregnated40 / 65 / 70 / 75 / 70 / 70 HS
Electrographitebase / epoxy / furan / babbitt / Cu / Sb impregnated30 / 40 / 40 / 40 / 40 / 40 HS

At a glance: SiC is hardest (HPSiC 93 HRA, SSiC 92, RBSiC 90); carbide next (87–91, YCN3 highest at 91); alumina 82–87 (99 ceramic harder than 95); carbon uses Shore — 40 HS base, up to 75 HS babbitt-impregnated; electrographite is softest at 30 HS base, 40 HS impregnated.

Pairing rules: when to go hard-on-hard

Hardness is a pairing basis, not "the harder the better". The textbook criteria: hard-on-hard (SiC/carbide or SiC/SiC) for crystalline, viscous and particle-laden media — hard faces resist abrasive cutting and resist particle embedding. A published slurry pump case cut failures sharply after changing to a SiC–carbide pair. Hard-on-soft (SiC vs carbon) suits clean media: the soft ring gives self-lubrication and run-in, the hard ring retains wear resistance — the economical standard configuration. Carbon impregnation also matters: babbitt 75 HS is soft and self-lubricating; metal impregnation resists erosion.

Filling the API 682 datasheet

Once faces are chosen, enter them accurately in the API 682 datasheet (Table A-27 for Series 1/2, Table A-28 for Series 3): distinguish buyer / seal vendor / default / to-fill / select ★ fields so a vendor default is not mistaken for a buyer requirement; submit all four data groups — seal, seal chamber, pump and fluid. Fluid particle content, temperature and pH feed back directly into whether the pairing is right. Write the grade and hardness (e.g. SSiC-A 92 HRA, YG8 89 HRA): "silicon carbide" or "carbide" alone is not enough, since sintering routes change hardness and corrosion resistance.

Factory tests linked to material choice

Spring-type seals: static pressure test + 5 h run. High-pressure vessel seals: gas-tightness + static + running. Medium/low-pressure vessel seals: static + 6 h run. Submersible pump seals: gas-tightness + static + 5 h run. Dry gas seals: visual + confirmation + static + dynamic tests. Changing face material does not exempt testing — a hard-on-hard pair has a different run-in leakage curve from a soft ring, so the full-duration test per the applicable standard is required.

About EGERSEAL: Jiaxing Egerseal Mechanical Seal Co., Ltd. (formerly Jiashan Xincheng Seal Parts Factory, established 2007) has nearly 20 years in mechanical seal R&D, manufacturing and repair, supplying zirconia, silicon carbide, ceramic, graphite, stainless steel and rubber seal parts matched to the medium. 45% of output is exported to 23 countries. MOQ 1 set, lead time 7–10 days.